Chilled Water Quality Limits

Most chiller failures we are asked to explain are not compressor failures. They are water failures that the compressor reported. Scale, corrosion and biological growth cost far more in lost efficiency and dead equipment than any mechanical fault, and almost all of it is decided by four numbers on a water test sheet that nobody reads until something breaks.

Closed loop vs open loop: different problem, different limits

The two circuits need to be treated as separate systems, because they fail in opposite ways.

A closed chilled-water loop has almost no make-up water, so dissolved solids stay put and the risks are corrosion and biological growth rather than scale. Oxygen enters once at commissioning and then only through leaks and faulty expansion tanks. Get the initial fill right and the loop is stable for years.

An open condenser-water loop loses water to evaporation and replaces it with make-up, which brings in hardness, chloride and alkalinity continuously. Evaporation leaves the dissolved solids behind, so the concentration cycles up until bleed-off removes them. This loop scales, and scale on a condenser tube is the single most expensive fouling problem in a plant.

Target limits for a closed chilled-water loop

ParameterTypical targetWhy it matters
pH8.0 – 10.0 (carbon steel); 7.5 – 9.0 with copper alloys presentBelow 7 is aggressive to steel; above 10 attacks copper and aluminium
ConductivityUnder 500 µS/cm at 25°CProxy for total dissolved solids and corrosion rate
ChlorideUnder 200 mg/L for 304; under 500 mg/L for 316; under 700 mg/L for duplexPitting and stress corrosion cracking — failure is sudden, not gradual
Total hardnessUnder 100 mg/L as CaCO₃Scale above roughly 60°C surface temperature
Total alkalinityUnder 200 mg/L as CaCO₃Buffers pH; high alkalinity plus hardness equals scale
Dissolved oxygenUnder 0.1 mg/L with inhibitor; not controlled without oneGeneral corrosion and pitting in carbon steel
IronUnder 1.0 mg/LRising iron means the loop is corroding somewhere
CopperUnder 0.1 mg/LRising copper means the coils or tube bundles are being attacked
Bacteria (planktonic)Under 10⁴ CFU/mLBiofilm insulates ten times better than scale and hides under-deposit corrosion
Glycol concentrationAs designed, ±2%Too weak freezes; too strong cuts heat transfer and raises pump power

These are working targets for industrial chilled-water systems, not a standard. Your water treatment supplier’s programme governs, and any figure here yields to a specific equipment warranty condition. Where the two conflict, the warranty wins — and it is worth reading the warranty’s water-quality clause before commissioning, not after a tube fails.

The three failures, and what each looks like

Scale. Calcium and magnesium carbonate deposit on the hottest surface, which is the tube wall on the refrigerant side of a condenser. A 1 mm scale layer on a condenser tube can cost 10–15% in compressor power, and the effect compounds because higher condensing pressure raises the compression ratio. It looks like a gradual efficiency loss that never quite recovers after a service. It is removed by chemical cleaning, prevented by softening or by running fewer concentration cycles.

Corrosion. Two distinct patterns. General corrosion thins the wall evenly and shows up as rising iron in the water test. Pitting is localised and fast, and it is what chlorides do to stainless steel: a pit that penetrates a 1.2 mm tube wall in eighteen months is entirely normal in water that “looks fine”. If your loop has 304 tubes and the chloride sits at 300 mg/L, the tubes are on a clock.

Biofilm. Slimy deposits, usually worst in the 20–45°C range and in low-velocity dead legs. Biofilm is a better insulator than scale and it creates the oxygen-depleted environment underneath that drives under-deposit pitting. It also harbours Legionella in open loops, which turns a maintenance issue into a regulatory one — an open condenser loop needs a documented water safety plan under ASHRAE 188 or the local equivalent, not just a biocide dose.

Velocity: the free variable

Water chemistry gets all the attention, but tube velocity decides as much. Below about 1 m/s in a horizontal tube you get settlement and under-deposit attack. Above the material’s limit you get erosion-corrosion at the inlet, which looks like a ring of thinning 100–200 mm into the tube.

MaterialWorking velocity window
Carbon steel1.0 – 2.0 m/s
Stainless 304/3161.2 – 2.5 m/s
Duplex 22051.2 – 3.0 m/s
Titanium grade 21.2 – 3.0 m/s (also the minimum for seawater settlement)
Copper-nickel 90/101.0 – 2.3 m/s; sulphide-polluted water needs the lower end

If the pump was sized for pressure drop and the resulting velocity is 0.6 m/s, no water treatment programme will keep that bundle clean. See tube material selection for how the choice is made and titanium for seawater duty for the marine case.

A monitoring routine that actually catches problems

  1. Monthly: pH, conductivity, chloride, hardness, iron, copper, and a dip slide for bacteria on open loops. Fifteen minutes and a test kit.
  2. Monthly: log the approach temperature (leaving chilled water minus evaporating temperature) and the condenser approach. A drift of 3–5°C over a season is a cleaning trigger, not a number to watch for another year.
  3. Quarterly: corrosion coupon or a removable test spool in the loop. This is the only way to measure actual metal loss rather than infer it from water chemistry. ASTM D1384 is the usual reference method.
  4. Annually: open one header and inspect a tube sample, or pull the plate pack on a plate unit. Photograph it with the date. Two years of photographs is a far stronger maintenance record than two years of invoices.

If you run glycol, add concentration and pH of the glycol itself to the monthly list — glycol degrades into organic acids, which drop the pH and turn a protective fluid into a corrosive one. That failure mode is common and almost never anticipated.

What this means for the equipment you buy

The water limits should drive the material choice, not the other way round. Three practical rules we apply at quotation stage:

Get the water analysis before the material is fixed. Chloride, hardness, pH, conductivity, and for open loops the make-up water as well. Quoting 304 because it is the default, on water nobody has tested, is how a warranty claim starts.

Size the velocity into the design. Tube count and pass arrangement set the velocity. A bundle designed for 2 m/s can always be run slower with a throttle, but a bundle designed at 0.6 m/s cannot be made to work.

Make cleaning possible. Removable bundles, drain points, and a plate pack that can be opened without dismantling the pipework. Sites clean equipment they can access.

Our shell and tube exchangers are built in eight materials from carbon steel to titanium, with the construction selected against the water analysis rather than a catalogue default. Send the water test with the duty and the selection comes back with the reason stated, in writing.

Frequently asked

What pH should chilled water be? 8.0–10.0 for a carbon steel loop, tightened to 7.5–9.0 if copper alloys are present. Below 7 the water attacks steel; above 10 it attacks copper.

How much chloride can 316 stainless take? Commonly quoted as under 500 mg/L at ambient temperature, but the real limit depends on temperature, oxygen and stagnation. Above 60°C, or in stagnant dead legs, the safe limit drops sharply — which is why marine and high-chloride duties go to duplex or titanium.

Is a 1 mm scale layer really significant? Yes. On a condenser tube it is commonly worth 10–15% in compressor power, and it raises the tube wall temperature, which accelerates further deposition.

Can I use potable mains water as make-up? You can, and it is often the right choice, but it brings hardness. Softened or demineralised make-up plus controlled cycles of concentration is cheaper than descaling a condenser every second year.

Save to list